Skip to content
UV-curePrimer

VTS40041

VTS40041 Clear UV-cure primer for vacuum coating, furniture (catalog: 100 %-solids clear UV primer)

Mix calculator

g
Thinner0.0 %

When: Only if the primer is too heavy for the gun/vacuum head at the current temperature; warm the material first.

Ratio 100 : 0.0

ComponentWeigh out
VTS40041part A500 g
VTL10000Thinner0.0 g
Total500 g

Covers roughly 5.56 m² at 90 g/m².

Pot life of the mix: n/a — single-component UV-cure, no hardener; stable until exposed to UV/daylight.

Ask about VTS40041

Answers are based on the VTS40041 data and the products it mixes with.

Questions and answers are stored to improve the assistant and prevent abuse; the question text is processed by Anthropic (USA). Privacy policy

Mixing matrix

  • VTL10000Thinner
    % by weight: 0–10 %catalog

    Only if the primer is too heavy for the gun/vacuum head at the current temperature; warm the material first.

    VTL10000 is a UV-reactive diluent that cures into the film (solids stay 100 %). Don't add ordinary solvents (S30/S31/S11): there's no flash-off before the lamp, so solvent gets trapped. Over 10 % costs hardness and sandability.

  • Thinner
    % by weight: 0 %schedule

    Moulding and picture-frame UV finish — per official schedule

    Schedule uses the primer neat at 100 g/m².

Percentages are per 100 parts of component A.

Characteristics

Solids
100official
Viscosity
approx. 40–80 s DIN4 at 20 °C (estimate, not published) srecommended
Pot life
n/a — single-component UV-cure, no hardener; stable until exposed to UV/daylightrecommended
Drying · Flash-off (min)
0catalog
Drying · Cure
UV lamp cure at 30 m/min line speed (moulding schedule, 100 g/m²)schedule
Drying · Sand or stack
0 hrecommended
Drying · Conditions
UV lamp; shop 18–25 °C
Thixotropy
norecommended

Colours

  • clear · clear

Application

Vacuum coater

Consumption
80–100 g/m² (official/catalog); 100 g/m² in moulding schedule g/m²official
Wet film
70–90 µmrecommended
Coats
1 coat → UV cure → brush sand K120/K150 → topcoatschedule
Flash-off
0catalog
Sanding between coats
Щётки шлифовальные K120, K150 после УФ-отвержденияschedule

Airmix (air-assisted airless)

Nozzle
0.28–0.33 mmrecommended
Pressure · fluid
12–20 barrecommended
Pressure · air
1–2 barrecommended
Spray viscosity
material warmed to 35–45 °C; VTL10000 up to 10 % only if still too heavyrecommended
Consumption
80–100 g/m²official
Coats
1 full wet coat (80–100 g/m²), UV cure, sandrecommended
Flash-off
0catalog
Recoat
immediately after UV cure and sandingrecommended
Sanding between coats
P240–P320 by hand/orbital, or K120/K150 brushes on profilesrecommended

Use it for profiles and parts where you need a cleaner fan. With 100 % solids, the material has to be warmed. For primers on large flat parts the methods page recommends airless. The film goes straight under the lamp with no wait. recommended

Airless

Nozzle
0.28–0.38 mmrecommended
Pressure · fluid
120–180 barrecommended
Consumption
80–100 g/m²official

For large flat parts. Coarser fan edges than airmix. recommended

HVLP

Nozzle
1.8–2.2 mmrecommended
Pressure · air
2–2.5 barrecommended
Pressure · fluid
0.8–1.5 barrecommended
Consumption
80–100 g/m²official

Samples and repairs only — HVLP struggles with solvent-free material, expect some orange peel, which sands out. recommended

Process and compatibility

Substrate preparation
Шлифование щётками K60, K80; при необходимости — краситель CTU 100% / CFS1 150% / S12 500%, 80 г/м², сушка 25–30 °C 5 минschedule
Sanding
K120, K150 brushes after UV cureschedule
Temperature and humidity
Shop 18–25 °C; material kept at constant temperature (warmed for spray); away from daylightrecommended

Storage

Safety: No manufacturer data. UV materials contain acrylate monomers (skin sensitisers): nitrile gloves, goggles, avoid skin contact; shield eyes and skin from UV lamps. When spraying use an A2P2 respirator.

Sources

Value tags: “official”, “dealer”, “catalog”, “schedule” are Technocolor data; “workshop” is from our own datasheets; “recommended” is our engineering estimate (hover to see the reasoning).

Not covered by the sources
  • No dealer page: t-colormarket.ru, woodonline.ru, lakokraska31.ru, ndom31.ru searched — not listed (dealer shop has no UV category)
  • No TDS/SDS PDF found (web search budget exhausted in this run)
  • Viscosity, density, gloss, hardness, chemical resistance not published (viscosity given only as a derived estimate)
  • UV cure dose (mJ/cm²) / lamp type & power for this primer not published — only 30 m/min line speed in the schedule
  • Manufacturer spray settings (nozzle, pressure, material temperature) not published — all derived
  • Shelf life, storage temperature, packaging unknown
  • Official page says application 'Распыление' while the name says vacuum application; catalog says spray, vacuum also possible — recorded both
  • Vacuum-coater application isn't on the official methods page. Vacuum settings are general practice only.